Why cast iron cracks, how to choose a machinable or non-machinable electrode, and the technique that gives a sound repair.
Pump bodies, gearbox housings, machine bases and engine blocks are often cast iron. They can be repaired by welding – but not with an ordinary mild-steel electrode.
Why cast iron is difficult
Cast iron has a lot of carbon. When it is heated and cooled quickly, the area near the weld becomes very hard and brittle, and shrinkage stresses crack it. A mild-steel electrode picks up carbon from the casting and the weld cracks too.
Choosing the electrode
| Type | Weld | Use for |
|---|---|---|
| Nickel (machinable) | Soft, can be drilled and machined | Repairs that need machining, threads, sealing faces |
| Nickel-iron | Stronger, still machinable | Thicker sections, ductile (SG) iron |
| Non-machinable (steel-based) | Hard | Low-cost filling of cracks and holes that won't be machined |
Technique for a sound repair
- Clean thoroughly – remove oil soaked into the casting; heat gently to burn it out if needed.
- Stop the crack – drill a small hole just past each end of the crack.
- Prepare a groove – grind or use a gouging electrode to open a U-groove.
- Use low current and small electrodes – 2.5 or 3.15 mm.
- Weld short runs – 25–40 mm at a time, and spread them out.
- Peen each run while hot with a round-nose hammer to relieve stress.
- Let it cool slowly – cover with dry sand or an insulating blanket. Never quench with water.
For larger castings, preheating the whole part evenly (often 250–400 °C) reduces cracking. Avoid heating just one spot.