Everything about covered welding electrodes – types and uses, current settings, how to weld, storage and fixing common defects.

Electrode Types

Which Electrode Does What?

Tap a type to see its coating, current, positions, uses and a practical tip.

E6013RutileGeneral purpose – mild steelMentrode – in production
CoatingRutile (titania), medium coated
CurrentAC or DC±; runs on low-OCV transformers
PositionsAll positions
Used forGates, grills, sheet metal, light structures, repair
TipEasiest electrode to use. Soft arc and self-releasing slag. Best choice for small workshops and thin to medium sections. View product →
E7016Basic low hydrogenCrack-resistant weldsMentrode – in production
CoatingBasic, potassium silicate
CurrentAC (OCV ≥ 70 V) or DC+
PositionsAll except vertical-down
Used forStructural steel, machinery, tanks, thick or restrained joints
TipMust be dry – re-dry at 300–350 °C. Keep a short arc. Good on AC transformers, unlike most E7018. View product →
E7018Basic low hydrogen · iron powderHigh strength, smooth beadMentrode – in production
CoatingBasic with iron powder (~110% recovery)
CurrentAC (OCV ≥ 70 V) or DC+
PositionsAll except vertical-down
Used forHeavy structures, pressure vessels, boilers, PEB, critical joints
TipThe workhorse for code and structural work. Re-dry before use and store in a holding oven at 100–150 °C. View product →
E6010 / E6011CellulosicDeep penetration, pipe rootMade to order / coming
CoatingCellulose (sodium for 6010, potassium for 6011)
CurrentE6010: DC+ · E6011: AC or DC+
PositionsAll positions, incl. vertical-down
Used forPipeline root and hot passes, rusty or dirty steel, site work
TipDigging arc with deep penetration and fast-freezing slag. Do not over-dry cellulosic electrodes – they need some moisture. Ask us →
E7024Rutile · iron powderHigh depositionMade to order / coming
CoatingThick rutile coating with iron powder
CurrentAC or DC±
PositionsFlat and horizontal fillets only
Used forLong fillet welds on thick plate, beams, ship building
TipVery high deposition rate. Drag the electrode lightly on the work for smooth, flat fillets. Ask us →
E8018-G / E9018-G / E10018-GLow alloy · low hydrogenHigh-strength steelsMade to order / coming
CoatingBasic, low hydrogen with alloying elements
CurrentAC or DC+
PositionsAll except vertical-down
Used forHigh-tensile steels, cranes, earthmoving and heavy equipment
TipMatch the electrode strength to the steel. Preheat and inter-pass control are often needed – follow your procedure. Ask us →
E7018-1Low hydrogen · low temperatureImpact toughness at −46 °CMade to order / coming
CoatingBasic with iron powder
CurrentAC or DC+
PositionsAll except vertical-down
Used forLow-temperature service, offshore and critical structures
TipSame handling as E7018, with extra impact toughness at low temperature. Ask us →
SS 308L / 309L / 316LStainless steelCorrosion resistantMade to order / coming
CoatingRutile or basic, stainless core
CurrentAC or DC+
PositionsMost positions (grade dependent)
Used forFood, dairy and chemical plants; 309L for joining stainless to mild steel
TipUse lower current than mild steel and short stringer beads to limit heat. Keep electrodes dry. Ask us →
Cast ironNickel / steel typesRepair & joiningMade to order / coming
CoatingSpecial coatings, machinable or non-machinable
CurrentAC or DC
PositionsFlat and horizontal mostly
Used forCracked housings, pump bodies, engine blocks, machine beds
TipWeld short lengths (25–50 mm), peen while hot and let cool slowly to avoid cracking. Ask us →
HardfacingWear resistant30 to 64 HRCMade to order / coming
CoatingAlloyed coatings for set hardness
CurrentAC or DC+
PositionsFlat and horizontal mostly
Used forBuild-up of shafts and rollers, crusher parts, buckets, wear plates
TipChoose hardness for the wear type. Use a buffer layer on cracked or high-carbon parts. Ask us →
Cutting & gougingSpecial purposeNo gas or air neededMade to order / coming
CoatingThick exothermic coating
CurrentAC or DC (high current)
PositionsAll positions
Used forCutting, piercing holes, removing defective welds, back-gouging
TipUse a high current and push the electrode with a sawing motion. Not for finished cut quality. Ask us →
Reading the Code

What Does E7018 Mean?

Every AWS A5.1 electrode code tells you its strength, positions and coating. Indian IS 814 codes describe the same electrode in a different format.

EElectrode for arc welding
70Minimum tensile strength 70,000 psi (about 490 MPa)
1Position: 1 = all positions, 2 = flat & horizontal, 4 = includes vertical-down
8Coating type and current (last two digits together)
Last digitsCoatingCurrent
E••10Cellulose, sodiumDC+
E••11Cellulose, potassiumAC, DC+
E••12Rutile, sodiumAC, DC−
E••13Rutile, potassiumAC, DC±
E••14Rutile, iron powderAC, DC±
E••15Low hydrogen, sodiumDC+
E••16Low hydrogen, potassiumAC, DC+
E••18Low hydrogen, potassium, iron powderAC, DC+
E••24Rutile, iron powder (flat/horizontal)AC, DC±
E••28Low hydrogen, iron powder (flat/horizontal)AC, DC+

AWS and IS 814 Side by Side

AWS A5.1IS 814
E6013ER4211
E7016EB5426H3X
E7018EB5426H3JX

In IS 814: E = covered electrode, R/B = rutile/basic coating, the next digits give strength and impact class, H3 = low hydrogen, J = iron powder (high recovery), X = radiographic quality.

The Strength Number – E60, E70, E80 and Up

The first two digits (three from E100 up) give the minimum tensile strength of the weld metal in thousands of psi (ksi). E60 and E70 electrodes are covered by AWS A5.1 (carbon steel); E80 and above are low-alloy electrodes under AWS A5.5 and always carry a suffix that shows the alloy.

CodeMin. tensileMetric (A5.1M / A5.5M)StandardTypical electrodes
E60xx60 ksi · 430 MPaE43xxAWS A5.1E6010, E6011, E6013
E70xx70 ksi · 490 MPaE49xxAWS A5.1E7016, E7018, E7024
E80xx80 ksi · 550 MPaE55xxAWS A5.5E8018-B2, E8018-C1, E8010-P1
E90xx90 ksi · 620 MPaE62xxAWS A5.5E9018-B3, E9018-G
E100xx100 ksi · 690 MPaE69xxAWS A5.5E10018-G, E10018-M
E110xx110 ksi · 760 MPaE76xxAWS A5.5E11018-G, E11018-M
E120xx120 ksi · 830 MPaE83xxAWS A5.5E12018-M

Higher strength is not always better: match the electrode to the strength of the steel you are welding. Over-matching hard, high-strength weld metal on mild steel can increase the risk of cracking.

What Comes After the Dash

Letters and numbers after the main code add extra requirements – alloy content, toughness or hydrogen level. Example: E8018-B2 H4R = 80 ksi, all positions, basic iron-powder coating, chromium-molybdenum alloy (B2), very low hydrogen (H4) and moisture-resistant coating (R).

SuffixMeaningExample
-1Improved toughness – impact tested at a lower temperature (−46 °C for E7018-1)E7018-1
A1Carbon-molybdenum (about 0.5% Mo) – for higher-temperature serviceE7018-A1
B1 – B9Chromium-molybdenum steels for boilers, pipes and high-temperature plant (B2 ≈ 1¼Cr-½Mo, B3 ≈ 2¼Cr-1Mo)E8018-B2, E9018-B3
C1 – C3Nickel steels for low-temperature toughness (C1 ≈ 2.5% Ni, C3 ≈ 1% Ni)E8018-C1, E8018-C3
D1 – D3Manganese-molybdenum steelsE9018-D1
P1Cellulosic pipeline electrode for high-strength line pipeE8010-P1
WWeathering steels – copper, nickel and chromium for corrosion resistanceE8018-W2
MMilitary-type specification with tight strength and toughness limitsE11018-M
GGeneral – meets the strength class; alloy content agreed between buyer and makerE8018-G, E10018-G
H4 / H8 / H16Diffusible hydrogen limit – max 4, 8 or 16 mL per 100 g of weld metalE7018 H4
RMoisture-resistant coating – passes a moisture absorption testE7018 H4R

Low-alloy grades such as E7018-1, E8018-G to E10018-G are available from us on order – see Made to Order. Always check the full requirements in the latest AWS A5.1 / A5.5 standards.

Electrode Finder

Which Electrode Should I Use?

Answer five quick questions and we'll suggest an electrode and size. For critical or code work, always follow your approved welding procedure.

WE SUGGESTE6013

3.15 mm

Mentrode E6013 – easy to use on any machine.

View this electrode →

A guide only. Not sure? WhatsApp us your job details and our team will advise.

How to Weld

Stick Welding in 8 Steps

Prepare the joint

Remove rust, paint, oil and moisture. Bevel plates over about 6 mm.

Choose the electrode

Pick grade and size for the steel, thickness and position.

Set the current

Use the packet range – lower for vertical and overhead.

Fix the earth clamp

On clean metal, close to the weld.

Strike the arc

Scratch like a match or tap lightly, then lift to the arc length.

Hold the arc

Arc length about the core diameter. Electrode 70–80° to the work.

Travel steadily

Keep an even speed so the bead is uniform and fuses both edges.

Finish & clean

Fill the crater before breaking the arc. Chip and brush the slag.

Storage & Re-drying

Keep Electrodes Dry

TypeRe-dryingHolding
Rutile – E6013100–150 °C, 1 h (only if damp)–
Low hydrogen – E7016, E7018300–350 °C, 1 h100–150 °C
Cellulosic – E6010, E6011Do not re-dryStore sealed

Storage Rules

  • Keep packets sealed until use, off the floor, below 60% humidity
  • Use the oldest stock first
  • Never use electrodes with cracked or damp coating
  • Return unused low-hydrogen electrodes to the oven
Troubleshooting

Common Defects & Fixes

ProblemLikely causeFix
Porosity (holes)Damp electrodes, rust/oil/paint, long arc, windRe-dry electrodes, clean the joint, keep a short arc, shield from wind
UndercutCurrent too high, wrong angle, travelling too fastLower current, pause at the edges, correct electrode angle
Excess spatterCurrent too high, long arc, damp electrodes, arc blowReduce current, shorten arc, use dry electrodes
Lack of fusionCurrent too low, travelling too fast, poor joint prepIncrease current, slow down, open up the joint gap and bevel
Slag inclusionsSlag not removed between passes, low currentChip and brush every pass, slightly higher current
CrackingHydrogen from damp electrodes, high-carbon steel, fast coolingUse low-hydrogen electrodes re-dried, preheat thick or high-carbon steel
Electrode stickingCurrent too low, poor strike techniqueRaise current, use a quick scratch or tap strike
Arc blow (wandering arc)Magnetic effects on DC near the earth clamp or endsMove the earth clamp, angle the electrode, or switch to AC

Welding Safety Guide

Electric shock, fumes, arc rays, fire, PPE and first aid – download the full guide.

FAQ

Questions Welders Ask

What is the difference between E6013 and E7018?

E6013 is a rutile, general-purpose electrode that is easy to use on mild steel. E7018 is a low-hydrogen, iron-powder electrode with higher strength and crack resistance for structural and critical work. E7018 must be kept dry and re-dried before use.

Can I use E7018 on an AC transformer?

Yes, if the machine has an open-circuit voltage of about 70 V or more. On low-OCV transformers, E7016 or E6013 will strike and run more easily.

How much current should I use?

A simple rule is about 30–40 A per mm of electrode diameter, then adjust within the range on the packet. Use the lower end for vertical and overhead welding. Try the calculator above.

Why do my welds have small holes?

That is porosity – usually from damp electrodes, a dirty joint or too long an arc. Re-dry low-hydrogen electrodes, clean rust and paint off the joint and keep the arc short.

Do I need to re-dry E6013?

Only if the electrodes have become damp. Re-dry at 100–150 °C for 1 hour. Do not over-bake rutile electrodes.

What does "low hydrogen" mean?

The coating is designed to put very little hydrogen into the weld. Hydrogen can cause cracking in thick or high-strength steel, so low-hydrogen electrodes like E7016 and E7018 are used for structural and pressure work.

Which size electrode should I choose?

Match the size to the plate: about 2.5 mm for thin sections up to 4 mm, 3.15 mm for 4–8 mm, 4.0 mm for 8–12 mm and 5.0 mm for thicker plate in the flat position. Use smaller sizes for vertical and overhead work.

Still Have a Question?

Our technical team will help you choose the right electrode and settings.

Items have been added to cart.
One or more items could not be added to cart due to certain restrictions.
Added to cart
Quantity updated
- An error occurred. Please try again later.
Deleted from cart
- Can't delete this product from the cart at the moment. Please try again later.