What tensile strength, elongation, impact and bend tests tell you about an electrode – and how to read a test certificate.
Every electrode classification – E6013, E7018 and the rest – comes with minimum test results the weld metal must achieve. Here is what those tests are and what the numbers on a test certificate mean.
Tensile test
A bar of weld metal is pulled in a Universal Testing Machine (UTM) until it breaks.
- Tensile strength – the highest load before breaking. "70" in E7018 means at least 70,000 psi (about 490 MPa).
- Yield strength – the load at which the metal starts to stretch permanently.
- Elongation – how much it stretches before breaking, a measure of ductility. Higher is better.
Impact (Charpy V-notch) test
A notched sample is broken with a swinging hammer at a set temperature, and the energy absorbed is measured in joules. It shows how tough the weld is and how well it resists brittle cracking, especially in the cold. E7018 must pass at −29 °C; E7018-1 at −46 °C.
Bend test
A welded strip is bent around a former. A good weld bends without cracking – a quick check of soundness and ductility.
Radiographic (X-ray) test
An X-ray of the weld shows hidden porosity, slag and cracks. Electrodes rated for radiographic quality give clean X-rays when used correctly – the "X" in IS 814 codes.
Chemical analysis
Checks that carbon, manganese, silicon, sulphur, phosphorus and any alloying elements are within limits.
Diffusible hydrogen
For low-hydrogen electrodes, measures how much hydrogen gets into the weld – shown by codes like H4, H8 and H16.