Moisture is the number one cause of porosity and cracking with E7016 and E7018. Here is how to store, re-dry and handle them on the shop floor.
Low-hydrogen electrodes such as E7016 and E7018 are chosen for one reason: crack-resistant welds. Their coatings are made to put very little hydrogen into the weld metal. But the coating also absorbs moisture from the air – and moisture is hydrogen. A damp low-hydrogen electrode loses the very property you paid for.
What goes wrong with damp electrodes
- Porosity – small gas holes in and under the weld bead, often worst at the start of each electrode.
- Hydrogen cracking – fine cracks that can appear hours after welding, especially in thick plate and higher-strength steel.
- Poor arc and more spatter – the arc becomes harsh and unstable.
Kerala's humid climate makes this worse. An opened packet left on the shop floor during the monsoon can pick up enough moisture in a few hours to cause problems.
How to store them
- Keep packets sealed until you need them. Vacuum-packed electrodes are available on request for extra protection.
- Store cartons off the floor, in a dry room, ideally below 60% humidity.
- Use the oldest stock first.
- Never use electrodes with cracked, chipped or swollen coating.
How to re-dry them
| Electrode | Re-drying | Holding oven |
|---|---|---|
| E7016, E7018 | 300–350 °C for 1 hour | 100–150 °C until use |
| E6013 | 100–150 °C for 1 hour, only if damp | Not needed |
No oven on site?
A portable electrode oven (quiver) that plugs into the welding machine or mains keeps electrodes at holding temperature next to the welder. For small jobs, buying in smaller packets – such as our 2.5 kg low-hydrogen packets – means less stock is exposed to air once opened.
Download the Mentrode datasheets for re-drying details for each grade.